Default Removing heat discoloration on stainless ??

Most people know you can remove heat bluing from stainless steel by polishing it. However for years I used to get a used machinery publication that had an advertiser than claimed they could remove the blue coloring electronically. They had a handle that had a small sock on the end that you were supposed to dip in some solution and then rub over the discolored area. The handle had a wire running to it. They made some strong clams on how many feet of weld it could clean per minute .

Is anyone familiar with this type of system ? Any leads or brand names or comments would be much appreciated. Thank you ~ John Buchtenkirch
__________________
John
Reply With Quote
  #2  
Old 08-19-2019, 08:40 PM
steve.murphy steve.murphy is offline
Member
 
Join Date: May 2009
Location: Brisbane, Australia
Posts: 650
Default

Hi John,
Just google electric stainless weld cleaner, you will find heaps.
__________________
Steve

ærugo nunquam dormit
Reply With Quote
  #3  
Old 08-20-2019, 01:20 AM
Jaroslav Jaroslav is online now
MetalShaper of the Month April 2020, September 2021, November 2022
 
Join Date: Dec 2012
Location: Czech Republic
Posts: 2,601
Default

Interresting.

https://www.youtube.com/watch?v=zXRKVhtQgZU
__________________
Jaroslav
Reply With Quote
  #4  
Old 08-20-2019, 06:28 PM
crystallographic crystallographic is offline
MetalShaper of the Month October '14 , April '16, July 2020, Jan 2023
 
Join Date: Dec 2010
Location: Western Sierra Nevadas, Badger Hill, CA
Posts: 4,388
Default electro-polishing stainless steel

see under "electro-polishing"
also "Acid dip"
__________________
Kent

http://www.tinmantech.com

"All it takes is a little practical experience to blow the he!! out of a perfectly good theory." --- Lloyd Rosenquist, charter member AWS, 1919.
Reply With Quote
  #5  
Old 08-21-2019, 02:57 AM
L ee L ee is offline
Member
 
Join Date: May 2016
Location: Carson Ca.
Posts: 11
Default

In the 70's I made stainless tanks & sinks for film developing.
To get the gold - brown weld marks off we would use Lionel train transformer wet rag with passivation acid backed by copper rod or sheet
Ground transformer to sink other positive wire to copper rod move rag backed by copper along weld worked great
__________________
L ee
Reply With Quote
  #6  
Old 08-21-2019, 02:26 PM
Gareth Davies Gareth Davies is offline
Member
 
Join Date: Aug 2012
Location: Staffordshire, England
Posts: 665
Default

I use a machine made by a company called Cougartron and the results are stunning. It’s very easy to use and the welds are clean but not left with the white staining that pickling paste leaves. There are, however, a few downsides.

1) Initial cost was high - starter kit was around £2.5k from memory.
2) Cleaning fluid is expensive - £100 for 5 litres
3) Carbon brushes are expensive - £135 for 10
4) It struggles to clean the discolouration from hot rolled material, the best results are on cold rolled or polished material.
5) Still creates an acidic steam/fumes during use.
6) Leaves a sticky residue that needs thorough cleaning with hot water afterwards.

Having said all that, we wouldn’t go back to pickling paste as the electronic cleaner is so much quicker and with better cosmetic results. It’s really for commercial shops but there’s no reason why a hobby welder shouldn’t own one, if you want professional looking work.

Here’s a link to Cougartron https://cougartron.com/int/weld-cleaning/
__________________
Gareth Davies
Reply With Quote
  #7  
Old 08-21-2019, 05:03 PM
galooph galooph is offline
Administrator
 
Join Date: Oct 2011
Location: Alsager, United Kingdom
Posts: 903
Default

There was a thread about this on a welding forum I'm on.

Several people reported success using 12V power supplies with the positive connected to the work, and the negative connected to a conductive brush, something like https://www.ebay.com/itm/Qty-1-Pure-...B/263542164351. For the cleaning solution, they used 1 part phosphoric acid to 3 parts water.

I've not tried it personally, as I rarely work with stainless, but the results looked impressive.
__________________
Dan Smith
https://galooph.com/
Reply With Quote
  #8  
Old 08-22-2019, 01:02 AM
lots2learn lots2learn is offline
Member
 
Join Date: Aug 2012
Location: Seattle WA
Posts: 136
Default

This is very easy to do with a small transformer, (low voltage). A screwdriver wrapped in fiberglass cloth with the acid is what I'm familiar with.
The use I have seen is to provide FDA compliant welds. Grinding causes places for bacteria to hide more so than the acid cleaning.
__________________
Greg
Reply With Quote
  #9  
Old 08-22-2019, 11:22 AM
John Buchtenkirch John Buchtenkirch is offline
MetalShaper of the Month October 2012
 
Join Date: Jul 2009
Location: Glen Cove, Long Island
Posts: 1,675
Default

Thanks guys, I didn’t even know what name to search for………….. saw the advertisements better than 10 years ago………. memory isn’t 100% anymore. Seems like getting a brush for my tig torch and cleaning chemicals might be the most $ensible way to go. At 71 I’m not really looking to spend a lot of $$$ on something I will not use every day. Every time I weld stainless I think I should know more about this but the new stainless sink Lil Franky & I made for the shop kinda reminds me every time I was my hands thru out the day. Polishing welds on inside corners is frustrating . ~ John Buchtenkirch
sink.jpg
__________________
John
Reply With Quote
  #10  
Old 08-22-2019, 06:40 PM
hillman hillman is offline
Member
 
Join Date: Jun 2009
Location: Kyabram,Victoria,Australia.
Posts: 100
Default

If you want to get rid of just the weld color, a stainless steel (only) wire brush while the weld is still hot is really good followed by a 3M Scotch-Brite paint stripper wheel when cold.
If it's a better finish you want a 3M Scotch-Brite light de-burring wheel will polish nice but don't try and use it as grinding wheel
__________________
"Hillman"
Reply With Quote
Reply

Thread Tools Search this Thread
Search this Thread:

Advanced Search
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off

Forum Jump

All times are GMT -5. The time now is 09:57 AM.

Powered by vBulletin® Version 3.8.11
Copyright ©2000 - 2024, vBulletin Solutions Inc.